Patios and Paving

Best Mortar Mix for Laying Patio Slabs

Which mortar mix is best for laying patio slabs? Compare sand and cement ratios, sharp vs building sand, semi-dry mixes, plasticiser and slurry primer.

On this page
  1. The short answer
  2. Sand and cement terms
  3. Mortar mix ratios by situation
  4. Why sharp sand rather than building sand
  5. How to mix bedding mortar
  6. What about a dry sand and cement mix?
  7. Laying the slabs
  8. Is a 20 mm slab thick enough?
  9. How much mortar do you need?
  10. Drying, curing and weather
  11. Pointing the joints
  12. Common mistakes
  13. FAQ

The short answer

For most garden patios laid with concrete flags or natural stone, the usual choice is a full bed of mortar made from sharp sand and general-purpose Portland cement, mixed to a damp, “semi-dry” consistency. Guides commonly suggest somewhere between 4:1 and 6:1 sharp sand to cement by volume. The exact figure matters less than three other things: the slab is fully supported, the mix is not too wet, and the base underneath is sound.

If your slabs or the supplier give laying instructions, follow those over any generic ratio. This is especially true for porcelain, which usually has specific requirements.

Sand and cement terms

Names differ between the UK and the US, which causes a lot of confusion when you are ordering materials.

  • Sharp sand (UK) is coarse, gritty sand. In the US, similar material is often sold as concrete sand or coarse sand.
  • Building sand or soft sand (UK) is finer and smoother. The US equivalent is closer to masonry sand.
  • General-purpose cement is ordinary Portland cement, sold in bags.
  • Ballast or all-in aggregate is a mix of sand and gravel used for concrete, not normally for bedding slabs.

Mortar mix ratios by situation

These are common starting points, not rules. Check the product’s own instructions.

Job Typical mix (by volume) Notes
Bedding concrete flags on a firm base Roughly 4:1 to 6:1 sharp sand to cement Mixed damp, laid as a full bed
Bedding natural stone Similar range Stone varies in thickness, so a full bed helps absorb the differences
Bedding porcelain Follow the manufacturer Often a full bed plus a slurry primer on the back of each slab
Pointing joints Around 3:1 to 4:1 building sand to cement Or use a purpose-made jointing compound; see what to use to fill gaps between paving slabs
Concrete for a base or edging haunch Commonly around 1:2:4 cement to sharp sand to 20 mm aggregate, or 1:5 with all-in ballast See concrete mix for laying kerbs and brick edging

A stronger mix is not automatically better. Very rich mortar can shrink and crack, and it will not make up for a poorly compacted base.

Why sharp sand rather than building sand

Sharp sand is coarser and more angular. It packs well, shrinks less, and gives a firmer bed under a slab. Building sand is finer and more workable, which is why it suits pointing and brick mortar, but it is generally considered less suitable for a thick bedding layer under paving.

How to mix bedding mortar

  1. Measure the sand and cement with the same bucket or shovel so the ratio stays consistent.
  2. Mix them dry until the colour is even, with no streaks of grey or yellow.
  3. Add water a little at a time. Aim for a damp, crumbly mix that holds together when squeezed in your gloved hand, without water running out of it.
  4. Mix only what you can lay in about an hour or so. Cement starts to set, and mortar that has begun to stiffen should not be “revived” with extra water.

Wear gloves, eye protection and a dust mask. Wet cement is alkaline and can cause skin burns, and cement dust irritates the eyes and lungs.

Plasticiser and washing-up liquid

Plasticiser makes mortar easier to work and helps it trowel more smoothly. Some DIYers add a small squirt of washing-up liquid (“fairy liquid”) as an improvised plasticiser, because it traps tiny air bubbles. The effect is hard to control, and too much can weaken the mix. A purpose-made plasticiser used as the label directs gives more predictable results.

What about a dry sand and cement mix?

You will often see advice to lay slabs on a “dry mix” of sand and cement. There are two different things people mean by this:

  • A semi-dry (damp) mix, which is the standard approach described above. It has just enough water to hydrate the cement and hold its shape.
  • A genuinely dry mix spread and relying on ground moisture, a sprinkle of water or rain to activate the cement. This is less reliable. The cement may not hydrate evenly, so the bed can end up weak in places, and bond to the back of the slab is poor. It is a particular risk with dense slabs such as porcelain.

Yes, you can mix sharp sand and cement, and that is what most bedding mortar is. The question is how much water goes in. If you want the convenience of a drier mix, a slurry primer on the back of the slab is commonly used to help the bond.

Laying the slabs

Full bed or spot bedding

A full bed of mortar under the whole slab is the more robust method. It supports the slab evenly, reduces rocking and cracking, and limits the voids where water and ants can collect. Spot bedding (a dab at each corner and the centre) is a quicker method that some people use for light garden paths, but a full bed is better practice, especially for patios used for furniture or for porcelain and thin slabs.

Bed thickness

Many guides suggest a bedding layer of roughly 30 to 40 mm. Much thicker than that, mortar is slower to cure and more prone to inconsistency. If you need to make up large level differences, fix them in the sub-base, not in the mortar. See how deep the sub-base should be for a patio.

Slurry primer

A slurry primer is a thin mix of cement and water (often with a bonding additive) brushed onto the back of the slab just before it goes down. It helps the mortar grip, and many porcelain suppliers require it. Follow the slab maker’s instructions for the exact product.

Setting each slab

  1. Trowel the mortar bed so it sits slightly proud of the final level.
  2. Lower the slab on and tap it down with a rubber mallet until it is level with your string line and has the correct fall for drainage. See what slope a patio should have.
  3. Keep joints consistent with spacers, typically somewhere around 5 to 10 mm for slabs, unless the supplier says otherwise.
  4. Occasionally lift a slab you have just laid to check the mortar has full contact with its back.

If you would rather lay on sand, see whether you can lay patio slabs on sand or need a mortar bed.

Is a 20 mm slab thick enough?

For porcelain, 20 mm is a very common outdoor thickness and is generally used on a full mortar bed over a solid, well-compacted base. For concrete or stone slabs, thinner ones are more fragile in transit and while being laid, and are more dependent on full support underneath. None of these are suited to vehicle traffic unless the supplier states they are. For driveways you need products specified for that load.

How much mortar do you need?

Work out the area, multiply by the bed thickness, and add a margin. For example, 10 m² at a 40 mm bed is 0.4 m³ of finished mortar. Dry sand and cement usually take up more volume than the finished mortar, so allow extra, in the region of 30 percent more, and round up. Bagged materials and bulk bags both have printed coverage estimates you can compare against.

Drying, curing and weather

Mortar “dries” and “cures” at different speeds. It may be firm enough to walk on lightly after a day or two, but cement keeps gaining strength for weeks, and 28 days is the usual benchmark for full strength. A thicker bed, such as a 2 inch (50 mm) layer, will generally take longer to firm up than a thinner one, and cool, damp or shaded conditions slow it further.

  • Avoid laying in frost or when frost is forecast.
  • In hot, sunny weather, mortar can dry too fast, so work in smaller sections and keep fresh work shaded or lightly damp.
  • Keep off new slabs for at least a day or two, and longer for heavy items.

Pointing the joints

Wait until the bedding has set before filling the joints. Which material suits best depends on how the slabs were laid and how wide the joints are. See what to use to fill gaps between paving slabs. Rigid mortar joints belong on rigid, mortar-bedded slabs. On flexible sand-bedded surfaces they tend to crack.

Common mistakes

  • Mixing the mortar too wet, so it slumps and shrinks.
  • Using building sand for the bedding layer.
  • Skimping on the compacted base. No mortar mix can fix this.
  • Spot bedding slabs that will carry furniture or foot traffic.
  • Laying without a fall, so water sits on the surface.

For more, see common mistakes to avoid when laying pavers. If you are laying over an existing slab, see laying paving slabs on an existing concrete base. If you are using small interlocking units rather than slabs, see interlocking concrete pavers.

FAQ

What is the ratio for mixing concrete for slabs?

If you mean the concrete for a base, a commonly quoted general-purpose ratio is about 1 part cement, 2 parts sharp sand and 4 parts 20 mm aggregate by volume, or around 1 part cement to 5 parts all-in ballast. If you mean the bedding mortar under paving, see the table above.

Is 10 mm or 20 mm aggregate better?

For general concrete such as bases, 20 mm aggregate is common. Smaller 10 mm aggregate suits thin sections and finer finishes. For bedding mortar you normally use sand only, with no aggregate.

Can I use bagged ready-mixed mortar?

Yes. Bagged bedding mixes are convenient for small jobs, though they cost more per square metre than mixing your own.

Keep exploring

Guides from other topics

All topics →